Max. Resistance to Continuous Heat
|
|
Thermoplastic
|
|
|
|
Max. Rest. Heat
|
|
Short Term
|
|
Material
|
Abv.
|
Tade Name
|
Filler
|
F
|
C
|
Cost/#
|
F
|
C
|
|
Polyimid
|
PI
|
Pyralin, Thermid
|
0%
|
600
|
316
|
|
600
|
316
|
|
|
|
|
40% Graphite
|
625
|
329
|
|
680
|
360
|
|
|
|
Kapton
|
50% glass
|
600
|
316
|
|
660
|
349
|
|
Polyphenylene Sulfide
|
PPS
|
Rayton, Fortron
|
0
|
250
|
121
|
|
275
|
135
|
|
|
|
|
40% glass
|
450
|
232
|
$ 3.90
|
490
|
254
|
|
|
|
Fortoron 1140L4
|
40% glass +
|
430
|
221
|
|
509
|
265
|
|
|
|
|
40% carbon
|
475
|
246
|
|
475
|
246
|
|
Polyether Ketones
|
PEK
|
Ultrapek, Kadel, Hostatec
|
0
|
300
|
149
|
|
330
|
166
|
|
|
|
|
30% glass
|
500
|
260
|
|
600
|
316
|
|
Polyetheretherketone
|
PEEK
|
|
0
|
275
|
135
|
|
300
|
149
|
|
|
|
|
30% glass
|
500
|
260
|
|
600
|
316
|
|
Polyamide Imide
|
PAI
|
Torlon
|
0
|
500
|
260
|
|
532
|
278
|
|
|
|
|
30% glass
|
500
|
260
|
|
539
|
282
|
|
|
|
|
30% Graphite
|
500
|
260
|
|
540
|
282
|
|
|
PEI
|
Ultem
|
0
|
350
|
177
|
$ 6.95
|
390
|
199
|
|
|
|
|
10% glass
|
375
|
191
|
|
405
|
207
|
|
|
|
|
20% glass
|
375
|
191
|
|
408
|
209
|
|
|
|
|
40% glass
|
380
|
193
|
|
415
|
213
|
|
Polyphthalamide
|
PPA
|
Amodel
|
0
|
|
|
$ 7.25
|
248
|
120
|
|
|
|
|
33% glass
|
410
|
210
|
|
530
|
277
|
|
|
|
|
45% glass
|
410
|
210
|
|
560
|
293
|
|
Polyester
|
PET
|
Valox, Rynite
|
0
|
180
|
82
|
$ 2.05
|
130
|
54
|
|
|
|
|
30%
|
400
|
204
|
|
405
|
207
|
|
Polycarbonate
|
PC
|
|
0
|
250
|
104
|
|
265
|
104
|
|
|
|
|
20% glass
|
280
|
138
|
|
290
|
143
|
|
|
|
|
40% glass
|
|
|
|
290
|
143
|
|
|
|
|
40% Graphite
|
275
|
135
|
|
290
|
143
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
Nylon 66
|
|
|
0
|
|
|
$ 2.20
|
190
|
88
|
|
|
|
|
33% glass
|
|
|
|
480
|
249
|
|
|
|
|
|
|
|
|
|
|
|
Nylon 66
|
|
Nylatron 1000
|
0
|
|
|
|
200
|
93
|
|
|
|
|
30% Graphite
|
|
|
|
470
|
243
|
|
|
|
|
40% Graphite
|
|
|
|
485
|
252
|
|
|
|
|
|
|
|
|
|
|
|
Nylon 66
|
|
Nylatron GS
|
0
|
|
|
|
210
|
99
|
|
|
|
|
30% glass
|
|
|
|
485
|
252
|
|
|
|
|
40% glass
|
|
|
|
490
|
254
|
|
Nylon 46
|
|
Stanyl TW241F12
|
60% glass
|
338
|
170
|
|
554
|
290
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
Thermalset
|
|
|
|
Max. Rest. Heat
|
|
Short Term
|
|
Material
|
Abv.
|
Tade Name
|
Filler
|
F
|
C
|
Cost/#
|
F
|
C
|
|
RTV Silicone
|
|
|
0
|
250
|
121
|
|
|
|
|
Silicone
|
|
|
Glass filled
|
500
|
260
|
|
500+
|
260+
|
|
Silicone
|
|
|
Graphite filled
|
450
|
232
|
|
480
|
249
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
Thermalset
|
|
|
|
Max. Rest. Heat
|
|
Short Term
|
|
Material
|
Abv.
|
Tade Name
|
Filler
|
F
|
C
|
Cost/#
|
F
|
C
|
|
Polyurethane
|
|
|
|
|
|
|
90
|
32
|
|
Styrene block Cop.
|
|
|
|
|
|
|
120
|
49
|
|
Copolymer
|
|
|
|
|
|
|
75
|
24
|
|
Olefin
|
|
|
|
|
|
|
90
|
32
|
|
Styrene-Ethylene Butylene-Styrens
|
|
Kraton G Eoprene G 964
|
|
266
|
130
|
|
|
|
|
|
|
Neoprene
|
|
150
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
Maximum Continuous Use Temperature ( MCUT) : The temperatur at which
physical strength decreased to 50% of its original value in 11.4 years
|
|
|
|
|
|
|
|
|
|
|
|
Short Term deformation temperature: at 264 lb/Sq inch
|
|